Complete Set of CAMPUS® Data, ASTM Data, Biopolymer Database, Application Database, Tradename Database, Literature Database, Toolbox.

Material datasheets available free. Online registration at: www.materialdatacenter.com

Material Data Center is a leading international information system for the plastics industry. Material Data Center offers a comprehensive plastics database, calculation tools, CAE interfaces, a literature database and an application database. For more information about Material Data Center visit www.materialdatacenter.com.

This is the free Material Data Center Datasheet of Ultramid® B3HG6 HSP BK23346 - PA6-GF30 - BASF

Material Data Center offers the following functions for Ultramid® B3HG6 HSP BK23346:
unit conversion, PDF datasheet print, comparison with other plastics, snap fit calculation, beam deflection calculation, CAE Interfaces

Check here, which other Ultramid B datasheets, application examples or technical articles are available in Material Data Center

Use the following short links to get directly to the properties of interest in this datasheet:
Any use of this information falls under the rules of our disclaimer.
Product Texts
Glass fiber reinforced and heat ageing resistant injection moulding grade with excellent flowability used e.g. for plastic parts in automotive or E&E industry.
The product offers a high purity regarding ionic and halogen containing compounds.
This helps to minimize potential corrosion processes and to protect sensitive electronic components.
The product has a LS coloration (Laser Sensitive) and can be marked with Nd:YAG lasers.
Processing/Physical Characteristicsdry / condUnitTest Standard
ISO Data
Melt volume-flow rate, MVR 104 / * cm³/10min ISO 1133
Temperature 275 / * °C -
Load 5 / * kg -
Molding shrinkage, parallel 0.2 / * % ISO 294-4, 2577
Molding shrinkage, normal 0.7 / * % ISO 294-4, 2577
Mechanical propertiesdry / condUnitTest Standard
ISO Data
Tensile Modulus 9300 / 5700 MPa ISO 527
Stress at break 170 / 100 MPa ISO 527
Strain at break 3.5 / 8.1 % ISO 527
Charpy impact strength, +23°C 82 / 89 kJ/m² ISO 179/1eU
Charpy impact strength, -30°C 58 / 53 kJ/m² ISO 179/1eU
Charpy notched impact strength, +23°C 9.9 / 15.5 kJ/m² ISO 179/1eA
Charpy notched impact strength, -30°C 7.9 / 7.5 kJ/m² ISO 179/1eA
Thermal propertiesdry / condUnitTest Standard
ISO Data
Melting temperature, 10°C/min 220 / * °C ISO 11357-1/-3
Temp. of deflection under load, 1.80 MPa 205 / * °C ISO 75-1/-2
Temp. of deflection under load, 0.45 MPa 220 / * °C ISO 75-1/-2
Electrical propertiesdry / condUnitTest Standard
ISO Data
Comparative tracking index - / 600 - IEC 60112
Other propertiesdry / condUnitTest Standard
Water absorption 6.35 / * % Sim. to ISO 62
Humidity absorption 2.1 / * % Sim. to ISO 62
Density 1350 / - kg/m³ ISO 1183
Material specific propertiesdry / condUnitTest Standard
ISO Data
Viscosity number 112 / * cm³/g ISO 307, 1157, 1628
Test specimen productionValueUnitTest Standard
ISO Data
Injection Molding, melt temperature 280 °C ISO 294
Injection Molding, mold temperature 80 °C ISO 294
Processing Recommendation Injection MoldingValueUnitTest Standard
Pre-drying - Temperature 80 °C -
Pre-drying - Time 4 h -
Melt temperature 260 - 290 °C -
Mold temperature 80 - 90 °C -
Diagrams
Stress-strain , Ultramid® B3HG6 HSP BK23346 (dry), PA6-GF30, BASF
Stress-strain , Ultramid® B3HG6 HSP BK23346 (cond.), PA6-GF30, BASF
Secant modulus-strain , Ultramid® B3HG6 HSP BK23346 (dry), PA6-GF30, BASF
Secant modulus-strain , Ultramid® B3HG6 HSP BK23346 (cond.), PA6-GF30, BASF
Tensile modulus-temperature , Ultramid® B3HG6 HSP BK23346 (dry), PA6-GF30, BASF
Tensile modulus-temperature , Ultramid® B3HG6 HSP BK23346 (cond.), PA6-GF30, BASF
Characteristics
Processing
Injection Molding
Delivery form
Pellets, Black
Additives
Lubricants
Special Characteristics
Heat stabilized or stable to heat
Applications
Automotive, Electrical and Electronical
Regional Availability
Other text information
Injection molding
PREPROCESSING
Pre/Post-processing, Pre-drying, Temperature: 80 °C
Pre/Post-processing, Pre-drying, Time: 4 h

PROCESSING
injection molding, Melt temperature, range: 260 - 290 °C
injection molding, Melt temperature, recommended: 280 °C
injection molding, Mold temperature, range: 80 - 90 °C
injection molding, Mold temperature, recommended: 80 °C
injection molding, Dwell time, thermoplastics: 10 min
Disclaimer
Copyright Altair Engineering GmbH. Altair Engineering GmbH assumes no liability for the system to be free of errors. The user takes sole responsibility for the use of this data under the exclusion of every liability from Altair Engineering GmbH; this is especially valid for claims of compensation resulting from consequential damages. Altair explicitly points out that any decision about the application of materials must be double checked with the producer of this material. This includes all contents of this system. Copyright laws are applicable for the content of this system.
Created: Source: www.materialdatacenter.com


Material Data Center is provided by M-Base Engineering + Software GmbH. M-Base Engineering + Software GmbH assumes no liability for the system to be free of errors. Any decision about the application of materials must be double checked with the producer of this material.

Additional information about this material, like producer contact address, etc. can be found at www.materialdatacenter.com. For access to this extra information a registration is requested. Free online registration is available.